尤物视频污,99热99热99超碰,精品久久久久女少妇,少妇精品无码,日B视屏久久香色,亚洲美女午夜福利av,国产美女被操,国产九九精品,国产久久色情

China Influence of Laser Cladding Process Parameters on Forming Quality - China Supplier
China Influence of Laser Cladding Process Parameters on Forming Quality - China Supplier China Influence of Laser Cladding Process Parameters on Forming Quality - China Supplier China Influence of Laser Cladding Process Parameters on Forming Quality - China Supplier China Influence of Laser Cladding Process Parameters on Forming Quality - China Supplier

Influence of Laser Cladding Process Parameters on Forming Quality

Price:Negotiable
Industry Category:
Product Category:
Brand: 國盛激光
Spec:


Contact Info
  • Add:西安市國家民用航天產(chǎn)業(yè)基地航天基地299號西安建工科技創(chuàng)業(yè)基地十號樓4層, Zip:
  • Contact: 段純
  • Tel:17392761868
  • Email:gsjgkj@163.com

Other Products

Description
Additional Information

Influence of Process Parameters on Forming Quality

1. Laser Power: The power directly affects the amount of powder that can be melted per unit time, influencing the cladding efficiency. When other working parameters are fixed, insufficient power may result in incomplete powder melting, pitting after polishing, inadequate bonding strength, and low coating hardness. Excessive power may cause overmelting of the melt track, leading to the appearance of oblique wrinkles on the surface.

2. Powder Feed Rate: After the powder stream interacts with the laser, it absorbs laser energy. A higher powder feed rate results in more absorbed laser energy. If the powder feed rate is too high, it may lead to insufficient laser energy, resulting in an unmelted coating, pitting after polishing, and failure to melt the substrate, preventing metallurgical bonding between the coating and substrate and causing coating peeling. A high powder feed rate leads to low powder utilization, while a low powder feed rate results in high powder utilization.

3. Scanning Speed: A higher scanning speed results in a thinner cladding layer, while a lower scanning speed results in a thicker cladding layer. Excessive scanning speed may prevent the formation of a molten pool on the substrate, leading to poor metallurgical bonding between the coating and substrate, slow cooling of the melt track, an excessively long red tail, and peeling. A lower scanning speed can improve coating hardness and powder utilization.

4. Step Over: A smaller step over results in a higher overlap rate and a smoother coating surface, while a larger step over results in a lower overlap rate and more pronounced coating streaks. The step over affects the dilution rate. A smaller step over results in less laser energy reaching the substrate, leading to a lower dilution rate. A larger step over results in more laser energy reaching the substrate, leading to a higher dilution rate.

5. Gas Flow Rate: The gas serves two purposes: transporting the powder and protecting the high-temperature coating from oxidation. Insufficient gas flow may cause powder clogging, while excessive gas flow may result in high powder velocity, significant bouncing, and low powder utilization. Generally, argon provides better protection for the coating than nitrogen, resulting in higher coating quality.

6. Nozzle Height: If the nozzle is too high, the powder dispersion increases, leading to low powder utilization. If it is too low, the nozzle is prone to powder adhesion during the cladding process.

Industry Category
Product Category
Brand: 國盛激光
Spec:
Stock:
Origin: China / Shaanxi / Xianshi
About Toocle.com - Partner Programme - Old Version
Copyright ? Toocle.com. All Rights Reserved.
(浙)-經(jīng)營性-2023-0192
ChatGlobal Chat Now 鄂州市| 资溪县| 盖州市| 淮滨县| 蓬莱市| 花莲县| 宁南县| 深泽县| 龙泉市| 伽师县| 平乡县| 阳春市| 武定县| 安庆市| 莲花县| 堆龙德庆县| 密云县| 太原市| 齐齐哈尔市| 清水县| 兴城市| 集安市| 出国| 邯郸县| 克东县| 高安市| 利川市| 青田县| 盱眙县| 格尔木市| 三穗县| 崇义县| 和政县| 南充市| 林口县| 大荔县| 江山市| 文山县| 奉贤区| 贺州市| 格尔木市|